摘要
To protect carbon/carbon (C/C) composites against oxidation, a SiC nanowire-toughened MoSi2-SiC coating was prepared on them using a two-step technique of chemical vapor deposition and pack cementation. SiC nanowires obtained by chemical vapor deposition were distributed random-orientedly on C/C substrates and MoSi2-SiC was filled in the holes of SiC nanowire layer to form a dense coating. After introduction of SiC nanowires, the size of the cracks in MoSi2-SiC coating decreased from 18 ± 2.3 to 6 ± 1.7 μm, and the weight loss of the coated C/C samples decreased from 4.53% to 1.78% after oxidation in air at 1500 °C for 110 h.
源语言 | 英语 |
---|---|
页(从-至) | 1879-1882 |
页数 | 4 |
期刊 | Corrosion Science |
卷 | 52 |
期 | 5 |
DOI | |
出版状态 | 已出版 - 5月 2010 |